IPC 7711A - 第82页
NOTES IPC-771 1A Number: 3.5.2 Revision: A Date: 10/03 Subject: SOT Removal P a g e2o f2 Copyright Association Connecting Electronics Industries Provided by IHS under license with IPC Not for Resale No reproduction or ne…

EQUIPMENT REQUIRED
Soldering system
Removal tips
Tweezer handpiece
MATERIALS
Flux
Flux-cored solder
Cleaner
PROCEDURE
1. Remove conformal coating (if any) and clean work area of any contamination,
oxides or residues.
2. Install removal tip into tweezer handpiece.
3. Start with tip temperature of approximately 315°C and change as necessary.
4. Apply flux to all lead/land areas. (See Figure 1.)
5. Clean residue from tips with damp sponge. (See Figure 2.)
6. Tin tips.
7. Lower tips over component and squeeze handpiece contacting ALL leads with
tips. (See Figures3&4.)
8. Confirm solder melt of ALL joints and lift component from PWB. (See Figures 4
& 5.)
9. Release component from tips by wiping on a heat resistant surface.
10. Prepare lands for component replacement.
Figure 1 Apply Flux
Figure 2 Clean Tips
Figure 3 Position Tips
Figure 4 Melt All Joints
Figure 5 Lift Component
7711A
Rework of
Electronic Assemblies
Revision: A
Date: 10/03
SOT Removal
Flux Application Method – Tweezer
Number: 3.5.2
Product Class: R, F, W, C
Skill Level: Intermediate
Level of Conformance: High
Material in this manual, IPC-7711 Rework of Electronic Assemblies, was voluntarily established by Technical Committees of
IPC. This material is advisory only and its use or adaptation is entirely voluntary. IPC disclaims all liability of any kind as to the
use, application, or adaptation of this material. Users are also wholly responsible for protecting themselves against all claims
or liabilities for patent infringement. Equipment referenced is for the convenience of the user and does not imply endorsement
by IPC.
Page1of2
Copyright Association Connecting Electronics Industries
Provided by IHS under license with IPC
Not for Resale
No reproduction or networking permitted without license from IHS
--``,``,-`-`,,`,,`,`,,`---

NOTES
IPC-7711A
Number: 3.5.2
Revision: A
Date: 10/03
Subject: SOT Removal
Page2of2
Copyright Association Connecting Electronics Industries
Provided by IHS under license with IPC
Not for Resale
No reproduction or networking permitted without license from IHS
--``,``,-`-`,,`,,`,`,,`---

EQUIPMENT REQUIRED
Soldering system
Hot air pencil
Hot air tip
Tweezers
MATERIALS
Flux-cored solder
Cleaner
Tissue/wipe
PROCEDURE
1. Remove conformal coating (if any) and clean work area of any contamination,
oxides or residues.
2. Adjust pressure output so hot air scorches a tissue from approximately 0.5 cm
away. (See Figure 1.)
3. Set heater temperature to approximately 425°C and change as necessary.
4. Install tip into the hot air pencil.
5. Apply flux to all lead/land areas. (See Figure 2.)
6. Position tip approximately 0.5 cm away from component. (See Figure 3.)
7. Direct hot air over component and heat until COMPLETE solder melt is
observed on ALL solder joints. (See Figure 3.)
8. Grasp component with tweezers and lift away from PWB. (See Figure 4.)
9. Release component from tweezers on a heat resistant surface.
10. Prepare lands for component replacement.
Figure 1 Adjust Air Pressure
Figure 2 Apply Flux
Figure 3 Melt All Joints
Figure 4 Lift Component
7711A
Rework of
Electronic Assemblies
Revision: A
Date: 10/03
SOT Removal
Hot Air Pencil
Number: 3.5.3
Product Class: R, F, W, C
Skill Level: Intermediate
Level of Conformance: High
Material in this manual, IPC-7711 Rework of Electronic Assemblies, was voluntarily established by Technical Committees of
IPC. This material is advisory only and its use or adaptation is entirely voluntary. IPC disclaims all liability of any kind as to the
use, application, or adaptation of this material. Users are also wholly responsible for protecting themselves against all claims
or liabilities for patent infringement. Equipment referenced is for the convenience of the user and does not imply endorsement
by IPC.
Page1of2
Copyright Association Connecting Electronics Industries
Provided by IHS under license with IPC
Not for Resale
No reproduction or networking permitted without license from IHS
--``,``,-`-`,,`,,`,`,,`---